Worked example

Four-fastener repair strip

Estimate a first-pass critical fastener load in a four-fastener repair strip.

Use the peak load as a screen. Actual fastener distribution is influenced by hole clearances and joint stiffness.

View live results

Inputs

Bolt group
N
Critical-hole geometry
mm
mm
mm
mm
Laminate allowables
MPa
MPa
MPa

Live results

SI
Bolt force
3,836.3 N
Bearing
409.86 MPa
Net tension
80.122 MPa
Min. margin
−0.011848
FailGeometry screen met · Bearing
Critical-hole load path
Plan view of a loaded hole, bearing contact, net section and shear-out planes wew/d 6.12e/d 3.27d
  • Bearing contact
  • Net section
  • Shear-out planes
Limit utilization101.2%
0%100% limit

Nominal stress and margin

ModeStressMargin
Bearing409.856 MPa−0.0118475
Net tension80.1222 MPa2.61947
Shear-out62.6838 MPa0.786745

Geometry and net-plane comparison

Width ratio w/d
6.11538
Edge ratio e/d
3.26923
Width margin w − 4d
11 mm
Edge margin e − 3d
1.4 mm
Net ligament e − d/2
14.4 mm
Net-plane shear
74.0017 MPa

Model and assumptions

Pbolt = P·factor/n · σbr = Pbolt/(dt) · σnt = Pbolt/[(w − d)t] · τso = Pbolt/(2et).

Treat P as the total group load. A factor of 1 gives equal sharing, and a larger factor raises the demand on the critical bolt. The strip is checked at a single hole with effective width w.

The screening geometry uses w/d ≥ 4 and e/d ≥ 3 as local design heuristics in the context of ASTM D5961 and MIL-HDBK-17. Test geometries and allowable data depend on the specific procedure and layup.

Margin is allowable divided by nominal stress, minus one. The comparison using e − d/2 shows a different net-plane stress. Use an allowable calibrated to that same stress convention before assigning a net-plane margin.

Scope. Preliminary in-plane static screening. Fastener strength, contact, bearing–bypass interaction, wedge splitting, fatigue and progressive damage need separate checks.

See calculation methods and references