9.5 mm high-traffic surface mix

Check a fine surface mix against the tighter high-traffic VFA band.

Design readout

Air voids
4
%
VMA
15.29
%
VFA
73.84
%
Eff. binder
4.87
%

Compacted mix phase blocks

Compacted mix phase blocksVOLUME FRACTIONSNMAS ⅜ inAIR4%EFF. BINDER11.3%BULK AGGREGATE84.7%VMA15.29%VFA73.84%DUST RATIO0.923
VMA contains air plus effective binder. Absorbed binder lies within the bulk aggregate volume.

Volumetric screen met

Dust ratio is 0.923. Screening limit is 0.6 to 1.2.

Calculation ledger
Aggregate by mix mass
94.1%
Effective aggregate SG
2.7265
Absorbed binder by aggregate mass
1.09%
Dust-to-binder ratio
0.923
Minimum design VMA
15%
Lower design VFA limit
73%
Upper design VFA limit
76%

Inputs

Changes update results

Binder and aggregate
%
%
Measured mix and design class

Work through this example

  1. Use Rice SG and binder fractions to calculate effective aggregate SG.
  2. Compute air and mineral void volumes from the compacted specimen.
  3. Correct binder for aggregate absorption and compare the volumetric screen.

The 9.5 mm high-traffic VFA screen is 73–76%. Change the traffic class to see the band change.

The screen uses the FHWA Superpave workbook limits and a ±0.1 percentage-point display band about 4.0% design air voids. Verify current agency mix specifications, gyrations, moisture susceptibility and any gradation exceptions.

Read the equations and sources