VMA contains air plus effective binder. Absorbed binder lies within the bulk aggregate volume.
Volumetric screen met
Dust ratio is 0.861. Screening limit is 0.6 to 1.2.
Calculation ledger
Aggregate by mix mass
95.3%
Effective aggregate SG
2.7136
Absorbed binder by aggregate mass
0.911%
Dust-to-binder ratio
0.861
Minimum design VMA
12%
Lower design VFA limit
67%
Upper design VFA limit
80%
Inputs
Changes update results
Work through this example
Use Rice SG and binder fractions to calculate effective aggregate SG.
Compute air and mineral void volumes from the compacted specimen.
Correct binder for aggregate absorption and compare the volumetric screen.
The low-volume 25 mm case uses a 67% lower VFA limit. Compare against a 19 mm selection.
The screen uses the FHWA Superpave workbook limits and a ±0.1 percentage-point display band about 4.0% design air voids. Verify current agency mix specifications, gyrations, moisture susceptibility and any gradation exceptions.
Superpave HMA Mix Volumetrics · US customary units
Volumetric screen met. Dust ratio is 0.861. Screening limit is 0.6 to 1.2.
Inputs
Binder by mix mass Pᵦ
4.7%
Binder SG Gᵦ
1.03
Bulk aggregate SG Gₛᵦ
2.65
No. 200 passing P₀.₀₇₅
3.3%
Rice maximum SG Gₘₘ
2.52
Compacted bulk SG Gₘᵦ
2.4192
Nominal max. size
25.0 mm · 1 in
Design traffic
< 0.3M ESAL
Results
Air voids
4%
Voids in mineral aggregate
13%
Voids filled with asphalt
69.23%
Effective binder by mix mass
3.83%
Aggregate by mix mass
95.3%
Effective aggregate SG
2.7136
Absorbed binder by aggregate mass
0.911%
Dust-to-binder ratio
0.861
Minimum design VMA
12%
Lower design VFA limit
67%
Upper design VFA limit
80%
The screen uses the FHWA Superpave workbook limits and a ±0.1 percentage-point display band about 4.0% design air voids. Verify current agency mix specifications, gyrations, moisture susceptibility and any gradation exceptions.