WeldMetalLab

ASME IX · EN 1011-1

Arc Welding Heat Input & Arc Energy

Compare net heat input or electrical arc energy with a WPS window and estimate wire deposition.

Engineering screening only. Verify the applicable code, material and qualified WPS/PQR before production use.

Inputs

Arc parameters
V
A
mm/min
mm
m/min
WPS limits
kJ/mm
kJ/mm

Live weld sheet

Updated from inputs
Arc and weld poolNet heat input 0.886 kJ/mm. Electrical arc energy 1.107 kJ/mm. Thermal efficiency 80 %. Arc power 5.72 kW NET HEAT0.886kJ/mmARC ENERGY1.107kJ/mmTHERMAL EFF.80%ARC POWER5.72kW ARC AND WELD POOL Travel 310 mm/minArc 1.107 kJ/mmGMAW NET HEAT WINDOWPASS
Pass · within screen

Net heat window · 0.5 kJ/mm to 1.25 kJ/mm on an efficiency-adjusted basis.

Result details

Net heat input0.886 kJ/mm
Electrical arc energy1.107 kJ/mm
Thermal efficiency80 %
Arc power5.72 kW
Energy used for check0.886 kJ/mm
Solid steel wire feed (mass)4.15 kg/h
Estimated net wire deposition3.82 kg/h
Entered window minimum0.5 kJ/mm
Entered window maximum1.25 kJ/mm
Distance to nearest bound0.364 kJ/mm

Calculation method

Arc energy = 60P / v · Net heat input = η × 60P / v

Use P in kW and travel v in mm/min for kJ/mm. Electrical power comes from V × I / 1,000 or from measured mean instantaneous V × I during the run. For waveform-controlled welding, use the acquisition method required by the governing procedure.

Planning thermal factors are SAW 1.00, GMAW/FCAW/SMAW 0.80 and GTAW 0.60. Use WPS bounds expressed on the same basis as the selected result. Wire figures use a solid-steel equivalent of 7,850 kg/m³. Tubular wire needs measured linear mass for a production estimate.

References

Worked examples