AWS D1.1 · EN 1011-2
H16 diffusible hydrogen sensitivity
The same mill chemistry is reviewed with an H16 consumable instead of a lower-hydrogen class.
Engineering screening only. Verify the applicable code, material and qualified WPS/PQR before production use.
Inputs
Live weld sheet
Updated from inputsPreheat floor · 105 °C working temperature vs 148 °C minimum.
Result details
| IIW carbon equivalent | 0.436 % |
|---|---|
| Ito–Bessyo Pcm | 0.258 % |
| Yurioka CEN | 0.427 % |
| Preheat screening minimum | 148 °C |
| Base-metal CET | 0.31 % |
| Controlling CET | 0.31 % |
| Diffusible hydrogen input | 16 mL/100 g |
| IIW weldability band | Elevated |
| Combined heat-path input | 58 mm |
| Raw Method B estimate | 148 °C |
| Minimum interpass screen | 148 °C |
| Working temperature margin | -43 °C |
Worked example
Starting inputs
- Combined thickness
- 58 mm
- Governing plate
- 31 mm
- Hydrogen class
- H16
- Net heat input
- 1.1 kJ/mm
- Specified WPS minimum
- 40 °C
- Working temperature
- 105 °C
Baseline results
- IIW carbon equivalent
- 0.436 %
- Ito–Bessyo Pcm
- 0.258 %
- Yurioka CEN
- 0.427 %
- Preheat screening minimum
- 148 °C
Use controlling CET 0.31 %, a 31 mm plate and 16 mL/100 g diffusible hydrogen. The Method B result is 148 °C and the entered WPS minimum is 40 °C. The higher value sets the screening floor.
Try it. Change H16 to H4. The estimated minimum changes while each chemistry index remains fixed.
Calculation method
Tₚ = 697·CET + 160·tanh(d/35) + 62·HD⁰·³⁵ + (53·CET − 32)·Q − 328
CE(IIW) = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15. Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B. CEN = C + [0.75 + 0.25 tanh(20(C − 0.12))]·[Si/24 + Mn/6 + Cu/15 + Ni/20 + (Cr + Mo + V + Nb)/5 + 5B].
The EN 1011-2 Method B screen uses CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40. When supplied, weld-metal CET plus 0.03 is checked against base-metal CET. Method B uses governing plate thickness, separate from the recorded combined thickness. Published model limits are CET 0.20–0.50, plate 10–90 mm, Q 0.5–4 kJ/mm and yield up to 1,000 MPa.