AWS D1.1 · EN 1011-2
Thick column plate with H8 consumables
A two-inch column plate meets a matching plate in a heavily built connection. Both pieces contribute to the recorded heat path.
Engineering screening only. Verify the applicable code, material and qualified WPS/PQR before production use.
Inputs
Live weld sheet
Updated from inputsPreheat floor · 199.4 °F working temperature vs 336.7 °F minimum.
Result details
| IIW carbon equivalent | 0.492 % |
|---|---|
| Ito–Bessyo Pcm | 0.296 % |
| Yurioka CEN | 0.498 % |
| Preheat screening minimum | 336.7 °F |
| Base-metal CET | 0.354 % |
| Controlling CET | 0.354 % |
| Diffusible hydrogen input | 8 mL/100 g |
| IIW weldability band | Elevated |
| Combined heat-path input | 4 in |
| Raw Method B estimate | 336.7 °F |
| Minimum interpass screen | 336.7 °F |
| Working temperature margin | -137.3 °F |
Worked example
Starting inputs
- Carbon · C
- 0.19 %
- Manganese · Mn
- 1.38 %
- Chromium · Cr
- 0.2 %
- Combined thickness
- 4 in
- Governing plate
- 2 in
- Hydrogen class
- H8
- Net heat input
- 40.64 kJ/in
Baseline results
- IIW carbon equivalent
- 0.492 %
- Ito–Bessyo Pcm
- 0.296 %
- Yurioka CEN
- 0.498 %
- Preheat screening minimum
- 336.7 °F
Use controlling CET 0.354 %, a 2 in plate and 8 mL/100 g diffusible hydrogen. The Method B result is 336.7 °F and the entered WPS minimum is 150 °F. The higher value sets the screening floor.
Try it. Use governing plate thickness for Method B. A recorded temperature below the derived floor calls for a procedure review.
Calculation method
Tₚ = 697·CET + 160·tanh(d/35) + 62·HD⁰·³⁵ + (53·CET − 32)·Q − 328
CE(IIW) = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15. Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B. CEN = C + [0.75 + 0.25 tanh(20(C − 0.12))]·[Si/24 + Mn/6 + Cu/15 + Ni/20 + (Cr + Mo + V + Nb)/5 + 5B].
The EN 1011-2 Method B screen uses CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40. When supplied, weld-metal CET plus 0.03 is checked against base-metal CET. Method B uses governing plate thickness, separate from the recorded combined thickness. Published model limits are CET 0.20–0.50, plate 10–90 mm, Q 0.5–4 kJ/mm and yield up to 1,000 MPa.
The preheat and interpass floors are the higher of the model result and the entered WPS minimum. The IIW bands at 0.40 and 0.50 are qualitative. Verify procedure assumptions, grade-specific limits, restraint, acceptable upper interpass temperature and the governing AWS requirements.