WeldMetalLab

AWS D1.1 · EN 1011-2

Thin plate outside Method B thickness range

Two 1/4 in plates are spliced with a measured start temperature and a chemistry report.

Engineering screening only. Verify the applicable code, material and qualified WPS/PQR before production use.

Inputs

Mill chemistry · mass %
%
%
%
%
%
%
%
%
%
%
Preheat conditions
in
Record the combined heat path for fit-up review. Method B uses governing plate thickness below.
in
kJ/in
%
Enter zero if unknown.
ksi
°F
°F

Live weld sheet

Updated from inputs
Preheated plate sectionIIW carbon equivalent 0.436 %. Ito–Bessyo Pcm 0.258 %. Yurioka CEN 0.427 %. Preheat screening minimum — CE(IIW)0.436%PCM0.258%CEN0.427%PREHEAT MIN— PREHEATED PLATE SECTION HAZH4 · diffusible HPlate 0.25 inH4 PREHEAT FLOORREVIEW
Review required

Preheat floor · The EN Method B floor is unavailable for these inputs.

  • Method B range exceeded. Check the material, thickness, yield strength and effective heat input.

Result details

IIW carbon equivalent0.436 %
Ito–Bessyo Pcm0.258 %
Yurioka CEN0.427 %
Preheat screening minimum—
Base-metal CET0.31 %
Controlling CET0.31 %
Diffusible hydrogen input4 mL/100 g
IIW weldability bandElevated
Combined heat-path input0.5 in
Raw Method B estimate—
Minimum interpass screen—
Working temperature margin—

Worked example

Starting inputs

Combined thickness
0.5 in
Governing plate
0.25 in
Hydrogen class
H4
Net heat input
21.59 kJ/in
Specified WPS minimum
68 °F
Working temperature
113 °F

Baseline results

IIW carbon equivalent
0.436 %
Ito–Bessyo Pcm
0.258 %
Yurioka CEN
0.427 %
Preheat screening minimum
—

The controlling CET is 0.31 %. A governing plate of 0.25 in is outside the Method B thickness range, so the example reports the chemistry indices and flags the temperature check for review.

Try it. The chemistry indices remain usable. The modeled preheat field stays blank because the governing plate is below the Method B range.

Calculation method

Tₚ = 697·CET + 160·tanh(d/35) + 62·HD⁰·³⁵ + (53·CET − 32)·Q − 328

CE(IIW) = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15. Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B. CEN = C + [0.75 + 0.25 tanh(20(C − 0.12))]·[Si/24 + Mn/6 + Cu/15 + Ni/20 + (Cr + Mo + V + Nb)/5 + 5B].

The EN 1011-2 Method B screen uses CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40. When supplied, weld-metal CET plus 0.03 is checked against base-metal CET. Method B uses governing plate thickness, separate from the recorded combined thickness. Published model limits are CET 0.20–0.50, plate 10–90 mm, Q 0.5–4 kJ/mm and yield up to 1,000 MPa.

The preheat and interpass floors are the higher of the model result and the entered WPS minimum. The IIW bands at 0.40 and 0.50 are qualitative. Verify procedure assumptions, grade-specific limits, restraint, acceptable upper interpass temperature and the governing AWS requirements.

References

More worked examples