WeldMetalLab

AWS D1.1 · EN 1011-2

Weld metal controls the CET calculation

A higher-alloy weld deposit has a known CET of 0.36. Its adjusted value governs the preheat model.

Engineering screening only. Verify the applicable code, material and qualified WPS/PQR before production use.

Inputs

Mill chemistry · mass %
%
%
%
%
%
%
%
%
%
%
Preheat conditions
mm
Record the combined heat path for fit-up review. Method B uses governing plate thickness below.
mm
kJ/mm
%
Enter zero if unknown.
MPa
°C
°C

Live weld sheet

Updated from inputs
Preheated plate sectionIIW carbon equivalent 0.383 %. Ito–Bessyo Pcm 0.213 %. Yurioka CEN 0.328 %. Preheat screening minimum 150 °C CE(IIW)0.383%PCM0.213%CEN0.328%PREHEAT MIN150°C PREHEATED PLATE SECTION HAZH4 · diffusible HPlate 35 mmH4 PREHEAT FLOORFAIL
Outside screen

Preheat floor · 140 °C working temperature vs 150 °C minimum.

Result details

IIW carbon equivalent0.383 %
Ito–Bessyo Pcm0.213 %
Yurioka CEN0.328 %
Preheat screening minimum150 °C
Base-metal CET0.265 %
Controlling CET0.39 %
Diffusible hydrogen input4 mL/100 g
IIW weldability bandLower
Combined heat-path input67 mm
Raw Method B estimate150 °C
Minimum interpass screen150 °C
Working temperature margin-10 °C

Worked example

Starting inputs

Carbon · C
0.12 %
Manganese · Mn
1.3 %
Chromium · Cr
0.1 %
Molybdenum · Mo
0.03 %
Vanadium · V
0.04 %
Nickel · Ni
0.1 %
Copper · Cu
0.08 %

Baseline results

IIW carbon equivalent
0.383 %
Ito–Bessyo Pcm
0.213 %
Yurioka CEN
0.328 %
Preheat screening minimum
150 °C

Use controlling CET 0.39 %, a 35 mm plate and 4 mL/100 g diffusible hydrogen. The Method B result is 150 °C and the entered WPS minimum is 25 °C. The higher value sets the screening floor.

Try it. The weld-metal CET plus 0.03 affects the thermal estimate. The reported base-metal chemistry indices still come from the mill sheet.

Calculation method

Tₚ = 697·CET + 160·tanh(d/35) + 62·HD⁰·³⁵ + (53·CET − 32)·Q − 328

CE(IIW) = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15. Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B. CEN = C + [0.75 + 0.25 tanh(20(C − 0.12))]·[Si/24 + Mn/6 + Cu/15 + Ni/20 + (Cr + Mo + V + Nb)/5 + 5B].

The EN 1011-2 Method B screen uses CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40. When supplied, weld-metal CET plus 0.03 is checked against base-metal CET. Method B uses governing plate thickness, separate from the recorded combined thickness. Published model limits are CET 0.20–0.50, plate 10–90 mm, Q 0.5–4 kJ/mm and yield up to 1,000 MPa.

The preheat and interpass floors are the higher of the model result and the entered WPS minimum. The IIW bands at 0.40 and 0.50 are qualitative. Verify procedure assumptions, grade-specific limits, restraint, acceptable upper interpass temperature and the governing AWS requirements.

References

More worked examples