WeldMetalLab

EN 1011-2 · Rosenthal

Weld Cooling Time t₈/₅ & HAZ Risk

Predict 800 °C to 500 °C cooling time, identify the 2D/3D heat-flow regime and screen HAZ hardening.

Engineering screening only. Verify the applicable code, material and qualified WPS/PQR before production use.

Inputs

Thermal inputs
°C
kJ/mm
mm
Screening window
s
s
%

Live weld sheet

Updated from inputs
HAZ cooling curvePredicted t₈/₅ 7.48 s. Governing heat flow 2D. Transition thickness 15.66 mm. Cold-cracking flag Lower T₈/₅7.48sHEAT FLOW2DTRANSITION15.66mmCRACK FLAGLower HAZ COOLING CURVE 800650500°Ctime →Start 100 °C2D · 7.48 s2D heat flow COOLING TIME WINDOWPASS
Pass · within screen

Cooling time window · 5 s to 25 s entered for this steel.

Result details

Predicted t₈/₅7.48 s
Governing heat flow2D
Transition thickness15.66 mm
Cold-cracking flagLower
2D cooling estimate7.48 s
3D cooling estimate5.98 s
Weld shape factor F₂0.9
Weld shape factor F₃0.9
Mean cooling rate40.11 °C/s
HAZ hardening tendencyLower
Distance to nearest time bound2.48 s

Calculation method

t₃ = (6700 − 5T₀)Q·Δ(1/T)·F₃ · t₂ = (4300 − 4.3T₀)10⁵(Q/d)²·Δ(1/T²)·F₂

Use temperature differences 500 − T₀ and 800 − T₀. Solve t₂ = t₃ for transition thickness. Below the transition, use the thin-plate 2D result. Above it, use the thick-plate 3D result. Seam factors are 1.0/1.0 for run on plate and 0.90/0.90 for butt welds. Corner and T-fillet 2D factors are midrange planning choices (0.80 and 0.55); both use 0.67 for 3D.

The qualitative hardening flag combines cooling below the entered minimum with CE(IIW) bands of 0.40 and 0.50. The cracking flag also adds hydrogen class and high restraint. Select cooling limits for the actual steel. Use grade-specific HAZ hardness, toughness and representative procedure tests for acceptance.

References

Worked examples