A 340 m² coated frame uses 32 kg zinc anodes in 0.65 Ω·m water. Design life is 16 years.

Inputs

SI units

Enter bare-metal design current density for each phase and its associated coating breakdown. Use final stand-off anode dimensions.

m²
yr
%
mA/m²
%
mA/m²
%
mA/m²
%
kg
m
m
V
Ω·m
Required mass
575.02 kg
Anodes needed
18
Output / anode
0.58 A
Capacity life
16.03 yr

Galvanic current field

Schematic
Galvanic current field (schematic, not to scale)Anode metalProtected steelConventional current through electrolyteDRIVING VOLTAGE0.18 VFINAL DEMAND8.16 AANODE OUTPUT0.58 A
Anode mass governs

Confirm final geometry, closed-circuit potentials, coating allowances and current distribution with the CP design basis.

Final demand ÷ modeled installed output

Calculation details

Alloy design capacity
780 A·h/kg
Initial demand
2.18 A
Mean demand
2.72 A
Final demand
8.16 A
Final single-anode resistance
0.3082 Ω
Count by net mass
18
Count by final current
14
Count for initial polarization
4
Installed net mass
576 kg
Total installed current output
10.51 A

Worked calculation

Starting values · SI
  1. Initial, mean and final current demands are 2.176, 2.72 and 8.16 A.
  2. Mean demand and 780 A·h/kg capacity give 575.01538 kg required alloy mass.
  3. Final resistance is 0.30824 Ω with 0.58397 A per anode. Count by mass is 18, by final current 14 and by initial current 4.

Compare the lower zinc capacity with its available driving voltage under the project’s closed-circuit potential assumptions.

Method and limits

  1. Estimate demand at three stages

    For each stage, demand = protected area × coating breakdown × corresponding bare current density. Convert percent to a fraction and mA/m² to A/m².

  2. Calculate net alloy mass

    M = mean demand × 8,760 × design years ÷ (capacity × utilization). Divide by net mass per anode and round up. Preset capacities are 2,000, 780 and 1,100 A·h/kg for aluminum, zinc and magnesium, respectively.

  3. Check final and initial current

    For a slender stand-off anode, R = ρ[ln(4L/r) − 1]/(2πL), with L ≥ 4r. Current per anode is ΔE/R. Round final demand divided by single-anode current up and select the larger of the mass and final current counts. The additional initial screen uses the same final geometry as a conservative check.